How to repair tension marks on precision piston rods

If the precision piston rod is pulled during operation and not treated in a timely manner, it can affect the use of the product in mild cases, and in severe cases, make the hydraulic cylinder unable to work. So how do we fix it? Local grinding and polishing methods are used to repair lighter pull marks; For heavier pull marks, welding repair and manual grinding are used to repair them.
Formation of pull marks: After disassembling the gas-liquid booster cylinder, it was found that a precision piston rod was severely pulled, with 6 pull marks arranged side by side. The main reason for the pulling injury is that after the dust ring becomes brittle and falls off in a block like manner, it not only loses its dust prevention effect, but also accumulates a lot of dust and impurities in the expansion joint, causing the piston rod to grind hard with impurities, resulting in pulling injury. The scars then scratch the rubber sealing components at the cylinder port, causing serious leakage of the hydraulic cylinder.
Repair requirements: The filler and base material should be combined stably and smoothly; The seasoning must be easy to use and easy to manually process; Manual processing should ensure that the diameter error of the precision piston rod is less than 0.06mm. After analysis, it was decided to use J422 welding rod as the filler. Because acidic welding rods are not sensitive to rust, oil stains, and moisture, and are not prone to generating hydrogenated pores; Good craftsmanship and easy operation; Beautiful welding seam formation; The material has moderate hardness and is easy to process by hand; Stable arc, large melting depth, and stable bonding with the base material.
Repair process:
1. Clean the area to be welded first, and then surround the pull marks with damp mud.
2. Select a welding rod with a diameter of 2.5mm, adjust the current of the welding machine to 120A, and use the straight line welding method to smoothly weld.
3. After all welding is completed, clean the mud and slag, and use a rough file to file along the circumference of the precision piston rod, leaving a machining allowance of 0.1-0.2mm.
4. A cylinder with an outer diameter of 185mm, an inner diameter of 125mm, and a length of 150mm is used as a model (the outer diameter of the piston rod is 125mm). It is sawn along the axis, with one being a rough model and the other being a precision model.
5. Apply a thin layer of red ink on the inner wall of the rough mold, and then rub the rough mold tightly against the area to be repaired along the axis several times. Then, use a fine file to remove the heavier red ink on the product. Repeat the filing process and leave a machining allowance of 0.04-0.07mm.
6. Then use a 320 mesh sand strip dipped in kerosene and fine mold to grind the product to the specified size.
7. Afterwards, dip the back of the sandcloth in kerosene for manual polishing. After measurement, the significant error is only 0.03mm.

香蕉日批视频| 午夜高清国产拍精品| 亚洲精品另类| 欧美一级片在线免费观看| 丁香五月草草B| 欧美色视频免费| 青青草国产去| 开心播播网婷婷在线| 国产爆乳一区| 六月天婷婷久久| 鲁丝片一区二区| 深水埗区| 日韩一级欧美| 国产三级片小视频| 成人 性调教在线网站| 亚洲永久中文字幕| 小泽玛利亚一区二区免费| 亚洲精品在线一二三区| 亚洲精品男人的天堂| www.ccyy.com| 天天夜碰日日摸日日澡性色AV | 欧美 日韩 国产一区| 国产精品久久在| 78M成人免费在线| 久久4精品久| 粉嫩虎白女毛片人体| 超碰图片大香蕉| 成全视频免费观看在线播放| 欧美一区三区专区在线| 天堂成人网站91| 久艹视频| 亚洲毛片在线视频| 日产a一a区二区| 日本毛高清免费黄视频| 国产日韩欧美综合| 欧美亚洲大片在线| 国产夫妻自拍一区| 丁香成人一区欧美成人| 极品黑丝自慰网站| 精品免费一区二区在线| 嗯啊久久|